Description
ERNiCu-7 has good strength and resists corrosion in many media, including seawater, salts, and reducing acids. And it can be used to overlay over carbon steel, provided a buffer layer of ERNi-1 is used for the first layer. This alloy is not age hardnable and when used to join Monel K-500 has lower strength than the base metal.. It can equivalent to: Oxford Alloy 60 FM 60 , Techalloy 418.
Applications
Dissimilar welding applications include joining alloys to Nickel 200 and copper-nickel alloys.
Widely used in marine applications because of its good resistance to the corrosive effects of seawater and brackish waters. Can be used for MIG overlay on steel after a first layer with nickel 208.
Product Details
Chemical composition
Grade |
Chemical composition(%) |
ERNiCu-7 |
C |
S |
P |
Si |
Mn |
Ni |
¡Ü0.15 |
¡Ü0.015 |
¡Ü0.02 |
¡Ü1.25 |
¡Ü4.0 |
62~69 |
Al |
Cu |
Others |
Ti |
Fe |
|
¡Ü1.25 |
Bal |
£¼0.5 |
1.5~3.0 |
¡Ü2.5 |
¡¡ |
Mechanical properties
Tensile Strength |
Yield Strength |
Elongation |
530 Mpa |
360 Mpa |
34% |
Welding paramaters
Process |
Diameter |
Voltage |
Amperage |
Gas |
TIG |
.045¡± (1.2mm) |
13-16 |
80-110 |
100% Argon |
1/16¡± (1.6mm) |
14-18 |
90-130 |
100% Argon |
3/32¡± (2.4mm) |
15-20 |
120-175 |
100% Argon |
1/8¡± (3.2mm) |
15-20 |
150-220 |
100% Argon |
MIG |
.045¡± (1.2mm) |
28-32 |
180-220 |
75% Argon + 25% Helium |
1/16¡± (1.6mm) |
29-33 |
200-250 |
75% Argon + 25% Helium |
SAW |
3/32¡± (2.4mm) |
28-30 |
275-350 |
Suitable Flux may be used |
1/8¡± (3.2mm) |
29-32 |
350-450 |
Suitable Flux may be used |
5/32¡± (4.0mm) |
30-33 |
400-550 |
Suitable Flux may be used |
Specifications
AWS 5.14 Class ERNiCu-7 / ASME SFA 5.14 Class ERNiCu-7 ASME II, SFA-5.14 UNS N04060 Werkstoff Nr. 2.4377 ISO SNi4060 Europe NiCu30Mn3Ti.
|